HOME > Á¦Ç°¼Ò°³> LAY Series ..
 
   

 

 

PC/ABS ALLOY : LAY 100
LAY 100 is the trade name of polycarbonate and ABS resins alloy. According to the various compositions of base polymers, a number of specific grades are available including high impact grade,
non-halogen type flame retardant and so on.

 

AUTOMOTIVE Instrument Panel, Consol Box, Glove Box Cover, Wheel Cover & Cap,
Back Mirror Housing
ELECTRICAL /
ELECTRONICS
Monitor Housing, Notebook Housing, Fax Frame, Cellular Phone Case,
CD-ROM Drive Tray and Main Frame, Switch
INDUSTRIAL Helmet, Terminal box, Electrical Tool Housing, Distributing Board Box,
Power tool component, Water meter Housing
 
¢Ã PHYSICAL PROPERTIES
PROPERTIES
ASTM
UNIT
PC/ABS ALLOY SERIES`
GRADE NO.
LPY100
LPY100H
LPY100M
LPY100F
LPY100FW
LAY100FN
SPECIFIC GRAVITY
D792
1.13
1.15
1.12
1.18
1.18
1.18
MELT FLOW INDEX
D1238
g/10min
6
8
5
20
16
13
IZOD IMPACT STRENGTH
D256
Kg¡¤cm
/cm
60
60
50
45
45
45
HEAT
DEFLE
CTION
TEMPER
ATURE
18.6kg/§²
D648
¡É
110
115
100
88
88
90
4.6kg/§²
D648
¡É
120
122
108
105
105
106
TENSILE STRENGTH
D638
Kg/§²
538
570
565
510
520
550
TENSILE ELONGATION
D638
%
90
90
100
85
85
50
FLEXURAL STRENGTH
D790
Kg/§²
800
810
820
820
830
880
FLEXURAL MODULUS
D790
Kg/§²
22,000
23,000
23,500
23,500
23,500
25,200
FLAMMABILITY (UL-94)
HB
HB
HB
V-0
V-0
V-0
 

 

¢Ã PROCESSING DATA (INJECTION MOLDING)

SPECIFICATION
UNIT
LPY 100 SERIES
DRYING TEMPERATURE
¡É
60 ~ 80
DRYING TIME
hrs
4 ~ 6
CYLINDER TEMPERATURE
REAR
¡É
200 ~ 230
MIDDLE
210 ~ 240
FRONT
220 ~ 250
NOZZLE TEMPERATURE
¡É
220 ~ 250
MOLD TEMPERATURE
¡É
50 ~ 80
SCREW SPEED
rpm
40 ~ 70